Pipe Wrinkling During Bending on Tube Bending Machine – Causes & Solutions
A heavy steel pipe curves through a hydraulic bending machine inside a working fabrication shop.
Wrinkling mostly occurs on the inner compression side of the bend. In rare cases, wrinkles appear at the pipe end or tail of the bending arc. Principle: The metal on the inner side is compressed during bending, and excess material accumulates to form wrinkles.
Problem: No wrinkle-resistant insert (anti-wrinkle block) on the inner bend, or improper position / worn anti-wrinkle block Answer: The compressed metal on the inner side accumulates without supporting restraint, causing wrinkles directly. Solution: Install an anti-wrinkle block matched with pipe diameter and wall thickness. Adjust its position so the front cutting point aligns with the bending tangent point. Replace worn blocks. Use wear-resistant copper or alloy material for anti-wrinkle inserts.
Problem: Insufficient mandrel extension or improper mandrel position (mandrelless bending / too short mandrel) Answer: The mandrel supports the inner pipe wall. If the extension length is inadequate, the inner wall of the bend lacks support, resulting in wall collapse and material stacking wrinkles. Solution: Increase mandrel extension appropriately, extend close to the bending tangent point (do not over-extend to avoid piercing the pipe wall). Use segmented ball-head mandrels. Mandrel is mandatory for thin-wall tubes.
Problem: Too thin pipe wall, or too small relative bending radius (small R/D ratio) Answer: Smaller bending radius brings heavier compression deformation on the inner side. Thin-wall tubes are highly prone to material stacking and wrinkling. Solution: Increase bending radius if product drawing permits. If the dimension is fixed, adopt higher-strength pipe material or use mandrel + anti-wrinkle block combined process.
Problem: Excessively fast bending speed Answer: At high bending speed, the inner metal cannot flow evenly, and local material piles up instantly to form wrinkles. Solution: Reduce bending angular speed and lower the bending parameter on CNC tube bender. Use low constant speed for thin-wall pipe bending.
Problem: Insufficient clamping force of clamping die, pipe slipping Answer: The workpiece slides inside the clamping die during bending, shifting the bending tangent point and disturbing metal flow, which creates wrinkles. Solution: Raise clamping pressure moderately. Check wear of clamping die teeth. Add anti-slip texture on clamping die. Ensure the clamping die arc fully matches the outer diameter of the tube.
Problem: Improper thrust of booster die (follow die) Answer: Insufficient booster thrust cannot feed material forward for compensation and causes inner material accumulation. Excessive thrust forcibly squeezes the pipe and generates ripples. Solution: Fine-tune booster thrust according to pipe size. The thrust should only assist smooth forward sliding without overload.
Problem: Defects of raw pipe material Answer: Out-of-round pipe, uneven wall thickness, oxide scale or inconsistent material hardness leads to uneven deformation during bending and causes wrinkling. Solution: Perform incoming inspection and reject tubes with excessive ovality or large wall thickness variation. Remove burrs and oxide scale before processing. Unify annealing state of raw tubes.
Problem: Inadequate lubrication Answer: High friction between mandrel and inner pipe wall hinders metal flow, and inner material accumulates to form wrinkles. Solution: Apply dedicated tube bending oil or emulsion to fully lubricate mandrel and pipe inner surface. Select suitable lubricant for steel pipe to reduce friction.
Problem: Excessive pressure of pressure die (guide die) Answer: Over-tight pressure die locks the pipe and prevents smooth sliding, resulting in compressed material accumulation and wrinkling on inner side. Solution: Reduce pressure die pressure. Ensure the pipe can slide freely without being locked.
Problem: Mismatch between die cavity arc and pipe outer diameter nswer: Oversized die cavity creates clearance between die and pipe. The pipe loses support and wrinkles inward during bending. Solution: Machine die cavity according to actual outer diameter of pipe. Replace bending dies with precise matching size to minimize clearance.
Quick Troubleshooting Sequence for On-site Commissioning
Check wear and matching of dies (anti-wrinkle block, clamping die, pressure die)
Adjust mandrel extension length
Tune pressure die force and booster thrust
Reduce bending speed and improve lubrication
Inspect incoming pipe quality